Thickness is the first number a packaging engineer specifies, and the first thing a buyer asks. This guide works in both directions: if you know the application, find the thickness range; if you know the thickness, find what it is normally used for.
Covers BOPP, BOPET, CPP, BOPA, BOPS, POF and PE films. All ranges are from our production specifications.
Last updated: 2026-11-28
The short answer: thickness by application
| Application | Film type | Thickness | Why this range |
|---|---|---|---|
| Bouquet / floral sleeve | BOPP flower wrap | 8–25 µm | Thinnest printable film; cost dominates |
| Thermal transfer ribbon base | BOPET | 3.5–4.5 µm | Must be thin for heat transfer |
| Capacitor dielectric | BOPP / BOPET | 3–10 µm | Thin film increases capacitance |
| Book cover lamination | BOPP thermal | 15–27 µm | Balances protection and cost |
| General printing / lamination | BOPP plain | 15–18 µm | Industry default starting point |
| Snack bag (print web) | BOPP metallized | 20–30 µm | Barrier + stiffness |
| Cigarette box wrap | BOPP cigarette | 20–25 µm | Tight shrink at low temperature |
| Adhesive tape base | BOPP tape base | 23–28 µm | Must survive coating tension |
| Ice cream / tub wrap | BOPP pearlized | 30–40 µm | Opaque + cold resistance |
| Bag film (heavy duty) | BOPP plain | 35–52 µm | Stiffness for standing bags |
| Frozen food / vacuum | BOPA nylon | 15–25 µm | Puncture resistance at low temp |
| Retort pouch (121 °C) | CPP retort grade | 50–80 µm | Must survive sterilisation |
| Pallet wrapping | PE stretch | 15–50 µm | Pre-stretch ratio dependent |
| Shrink bundle / multipack | POF shrink | 12–25 µm | Balanced shrink force |
| Solar backsheet base | BOPET | 50–250 µm | Electrical insulation + weathering |
| Electrical insulation | BOPET | 100–350 µm | Dielectric strength |
Reading the table backwards: what a given thickness can do
3–6 µm — ultra-thin
Only BOPET and capacitor-grade BOPP reach this range.
- BOPET 3.5–4.5 µm — thermal transfer ribbon (TTR) base film. The film must be thin enough for print head heat to transfer wax/resin, and stable enough not to deform. This is a precision product, not a packaging film.
- BOPP / BOPET 3–6 µm — capacitor dielectric. Thin film means more electrode area per volume, which raises capacitance. Requires very tight thickness tolerance (±3 % or better).
At this range, handling is difficult and yields are low. Expect significantly higher cost per kilogram.
8–12 µm — floral and light lamination
BOPP flower wrap starts at 8 µm. This is the thinnest practical printable packaging film. Below 10 µm the film becomes hard to control on standard converting lines — it wrinkles, static becomes a problem, and tension control gets critical.
Use 10–12 µm when the pack is small, the wrap is decorative, and cost per unit matters more than stiffness.
15–18 µm — the workhorse range
This is where most BOPP printing and lamination sits. 15 µm and 18 µm are the two most common specifications in the industry.
- 15 µm — carton window, light lamination, general print
- 18 µm — standard print web, booklet cover lamination, label face stock
BOPP plain at 15–18 µm gives haze ≤ 1.5 %, gloss ≥ 85 GU, and surface tension ≥ 38 mN/m — printable on solvent, water-based and UV systems without pretreatment beyond the supplied corona.
BOPP thermal lamination at 15–18 µm is the standard for offset-printed sheets. The EVA hot-melt layer bonds at 90–110 °C, 8–15 MPa, 30–60 m/min.
20–30 µm — food packaging core
The largest volume band. Almost every snack, biscuit, confectionery and coffee pack uses a film in this range as the print/barrier web.
- BOPP metallized 20–30 µm — moisture barrier plus light barrier, mirror finish. MVTR drops sharply compared with clear BOPP because of the aluminium layer.
- BOPP heat sealable 20–25 µm — where the pack is formed on FFS equipment and needs a seal layer.
- BOPP cigarette 20–25 µm — tight shrink at 120 °C, high gloss, controlled COF so packs slide in the cartoner.
- BOPET 12 µm — the standard polyester lamination web. Stronger and more heat-resistant than BOPP, used where the pack needs puncture resistance or high-temperature filling.
30–52 µm — stiffness and barrier
Above 30 µm, film cost rises faster than barrier benefit for most food packs. This band is chosen for mechanical reasons:
- BOPP pearlized 30–40 µm — ice cream tubs, soap wrap. The opacity hides contents and the density (0.55–0.75 g/cm³) means more area per kilogram than clear BOPP.
- BOPP plain 35–52 µm — bag film, standing pouches, heavy-duty overwrap.
- CPP 30–50 µm — sealant web in retort and stand-up pouch structures.
- BOPA 15–25 µm — note that nylon is specified thin because its value is puncture strength, not thickness. A 15 µm BOPA outperforms a 40 µm BOPP on puncture.
50–350 µm — technical films
BOPET above 50 µm stops being a packaging film and becomes an industrial film:
- 50–125 µm — solar PV backsheet base, flexible circuit carrier
- 100–250 µm — electrical insulation, motor slot liner
- 250–350 µm — heavy electrical insulation, membrane switch spacer
These are specified on dielectric strength and dimensional stability, not on print or seal.
Thickness vs. cost: where the money goes
Cost per kilogram is roughly flat across a product family — a kilogram of 12 µm BOPP costs about the same as a kilogram of 40 µm BOPP. But cost per square metre scales almost linearly with thickness.
The practical consequence: halving thickness roughly halves your material cost per pack, provided the thinner film still meets the mechanical and barrier requirement. This is why downgauging is the single biggest cost lever in flexible packaging — and why the thickness decision deserves more attention than the grade decision.
Worked example. A pack that uses 25 µm BOPP can often move to 20 µm if the stiffness requirement is met by the pack format rather than the film. That is a 20 % material reduction with no change in supplier or grade.
The limit is usually one of:
- Seal integrity (thinner film seals faster but tears more easily at the seal edge)
- Machine runnability (below about 12 µm, tension control and static become difficult)
- Barrier (thinner film has proportionally less barrier per unit area)
- Stiffness (standing pouches need a minimum bending stiffness)
Thickness by film type at a glance
| Film | Common range | Thinnest we supply | Thickest we supply |
|---|---|---|---|
| BOPP plain | 15–30 µm | 10 µm | 52 µm |
| BOPP heat sealable | 18–30 µm | 15 µm | 52 µm |
| BOPP pearlized | 25–40 µm | 18 µm | 40 µm |
| BOPP metallized | 20–30 µm | 20 µm | 75 µm |
| BOPP matt | 12–18 µm | 12 µm | 18 µm |
| BOPP thermal lamination | 20–27 µm | 15 µm | 37 µm |
| BOPP tape base | 23–28 µm | 23 µm | 28 µm |
| BOPP anti-fog | 20–45 µm | 20 µm | 45 µm |
| BOPP cigarette | 20–25 µm | 20 µm | 25 µm |
| BOPP flower wrap | 8–25 µm | 8 µm | 50 µm |
| BOPET clear | 12–50 µm | 4.5 µm | 350 µm |
| BOPET metallized | 4.5–12 µm | 4.5 µm | 12 µm |
| BOPET TTR base | 3.5–4.5 µm | 3.5 µm | 4.5 µm |
| BOPA nylon | 12–25 µm | 12 µm | 80 µm |
| BOPS | 27–39 µm | 27 µm | 39 µm |
| CPP / GCPP | 20–80 µm | 20 µm | 80 µm |
| VMCPP | 20–40 µm | 20 µm | 40 µm |
| POF shrink | 12–25 µm | 12 µm | 50 µm |
| PVDC K-film | 20–32 µm | 20 µm | 32 µm |
| PE stretch | 15–50 µm | 15 µm | 50 µm |
Tolerance: the number that is often missing
A thickness specification without a tolerance is incomplete. Two suppliers quoting "20 µm" can differ by a factor of two in actual process capability.
Our standard tolerances:
| Thickness range | Tolerance | Measurement |
|---|---|---|
| 3–10 µm | ± 3 % | β-ray, online |
| 10–30 µm | ± 3 % | β-ray, online |
| 30–75 µm | ± 3 % | β-ray, online |
| BOPET technical | ± 2 % | Micrometer, offline |
For capacitor and TTR grades, tolerance is tighter and should be specified explicitly. Ask for the actual capability study (Cpk) if the film feeds an automated process.
Frequently asked questions
What does "µm" mean and how does it relate to "gauge"? µm is micrometre (micron), 1/1000 mm. Gauge is a legacy unit: 1 gauge = 0.254 µm, so 100 gauge ≈ 25.4 µm. Most of the world now specifies microns; the US still uses gauge in some segments. 80 gauge = 20.3 µm, 120 gauge = 30.5 µm.
How do I convert thickness to yield (m²/kg)? Yield = 1,000,000 / (thickness in µm × density in g/cm³). For BOPP at 0.91 g/cm³ and 20 µm: 1,000,000 / (20 × 0.91) ≈ 54,945 m² per tonne, or about 55 m²/kg. Pearlized BOPP at 0.65 g/cm³ and 35 µm: 1,000,000 / (35 × 0.65) ≈ 43,956 m²/t ≈ 44 m²/kg.
Can I get the same grade in a different thickness? For most BOPP and BOPET grades, yes — thickness is set at the extrusion line and can be adjusted within the range shown above. Very thin and very thick ends of each range carry longer lead times and higher minimums.
Why is BOPA supplied much thinner than BOPP for the same job? Nylon's value is puncture and tear resistance, which it delivers at low thickness. A 15 µm BOPA film has better puncture strength than a 40 µm BOPP film. Specifying nylon thick wastes money.
What thickness for a stand-up pouch? The structural layer is usually 12 µm BOPET (stiffness, print, heat resistance), the barrier layer 20–30 µm metallized BOPP or metallized BOPET, and the sealant 50–80 µm CPP or PE. Total structure 90–130 µm. The film thickness alone does not determine pouch stiffness — the lamination structure does.
Does thinner film mean lower barrier? Yes, roughly proportional for a homogeneous film: halving thickness roughly doubles transmission rate. Metallized films behave differently because the barrier comes from the aluminium layer, which is a fixed thickness regardless of base film — so a thinner metallized base loses less barrier than you would expect.
Request a thickness recommendation
Send us the application, pack format, filling temperature and annual volume, and we will confirm the thinnest film that meets the requirement — which is usually the cheapest one that works.
- Email: sale@boppfilmsale.com
- Phone / WhatsApp: +86 189 1965 9471
- Technical data sheets: Film specifications
- Grade comparison: BOPP selection guide